Quick answer: an OTR or WVTR figure is only usable with five things attached: temperature, relative humidity, test gas, thickness (or package) basis and test method. Put all five in every barrier spec, and treat a dry-condition OTR for EVOH or polyamide as a best case, not a forecast of what the pack will do on a humid shelf.
This piece rests mainly on instrument makers (Ametek Mocon and Labthink, who sell permeation testers), a packaging distributor, patent test-method sections and academic papers. Independent data is noted where it exists. Figures below are typical values from those sources, not specifications for any grade.
What the number is, and how units trip people up
OTR is the amount of oxygen that diffuses through a material per unit of time, commonly expressed in cm3/m2/day. WVTR is the same idea for water vapour, in g/(m2 day). Both are measured on a specific sample, so they describe that film at that thickness, not the polymer in general.
Imperial values still turn up on data sheets. One converter page gives the example that 0.6 cc/100 in2/day is the same as about 9.3 cc/m2/day. Pressure units also vary: many sheets say per atm, others per bar, and the two differ by about 1.3 percent (1 atm = 1.01325 bar), which only matters when you’re comparing close values.
Free tool: the unit converter handles gsm, microns, gauge and density, which helps when a sheet quotes thickness in gauge and your spec uses micrometres.
Which method produced the number
Start by checking the method name. Common OTR methods are ASTM D3985 (coulometric), ASTM F1927 or ISO 15105-2, and the Wikipedia overview of OTR methods also lists ASTM F1307 for packages, F2622 for various sensors and F3136 for dynamic accumulation.
| Method | Measures | Detector | Conditions often used |
|---|---|---|---|
| ASTM D3985 | OTR of film or sheet | Coulometric | One patent test section states 100% O2, 0% RH, 23 C, 760 mmHg (patent 9,181,460); other patents run it at 85% RH |
| ASTM F1927 | OTR at a controlled RH | Coulometric | RH set by the requester, which is why it appears in EVOH and PVdC work (patent 7,416,767) |
| ASTM F1307 | OTR of whole dry packages | Coulometric | Outside of the pack challenged with 20.9% oxygen in most cases, inside swept with dry nitrogen |
| ASTM F1249 / ISO 15106-2 | WVTR of film or package | Modulated infrared | One side at usually 90% or 100% RH; 38 C is the usual temperature on supplier pages |
| ASTM E96 (gravimetric) | Water vapour permeability | Weight change | An EVOH review used 38 to 40 C at 0 and 90% RH (Taylor and Francis) |
Two caveats from the standards themselves. Mocon notes the output is a rate-versus-time graph, which is how you verify equilibrium, and that tests can run from a few hours to a few weeks. And the F1307 text says gas transmission is not the sole determinant of package performance, so additional tests are needed to correlate it with real packs. Check the current edition of any standard before you cite it in a spec; a standards catalogue page lists F1307-20 as the most recent edition as of its listing.
Writing a barrier spec in six steps
- Name the quantity and unit. Say OTR in cm3/(m2 day) or permeability in cm3 µm/(m2 day atm), and state whether it is per atm or per bar.
- State the conditions. Temperature, RH on the test side and the carrier side, test gas concentration, and the method with its edition.
- State the level. Material (film or sheet, D3985) or package including seals and closure (F1307). A film that passes can still fail as a pack.
- Ask for the equilibrium plot. A single number without the rate-versus-time curve hides whether the film had stabilised, which matters most for hygroscopic layers.
- Ask for typical and worst case. Request sample count and lot-to-lot spread, not a single mean.
- Add a second test point at your real storage condition. If the product sits at 23 C and 75% RH, a 0% RH number alone doesn’t describe it.
What moves the number
| Factor | What happens | Reported size | What to do in the spec |
|---|---|---|---|
| Humidity (EVOH, PA) | Barrier improves slightly at low RH, then worsens as water plasticises the polymer | EVOH with 32 mol% ethylene, 15 µm: 0.01 to 0.05 mL mm/(m2 day atm) at 20 C as RH rises from 0 to 85% | Test at the RH the EVOH layer will actually see |
| Ethylene content | More ethylene means higher permeability | At 20 C and 65% RH, ISO 14663-2: 6 (EVOH32) versus 38 (EVOH44) cm3 µm/(m2 day atm) | State the grade, not just “EVOH” |
| Temperature | Permeation rises with temperature, following an Arrhenius curve | See our calculation below | Quote temperature with every number |
| Thickness | Thinner homogeneous film passes more gas | For PE films, OTR rose linearly as thickness fell | Give OTR at the actual thickness and the layer stack |
| Coating defects | Inorganic coatings leak through flaws | Oxygen permeation in oxide-coated films was controlled by macro-defects in the oxide layer | Add flex and handling tests (for example ASTM F392) |
| Batch variation | Nominally identical films differ | A study of PE modified atmosphere films from three suppliers reported bag-to-bag variation as high as 74.2% for supplier C | Ask for spread, test several lots |
Humidity and the EVOH sandwich
The mechanism is documented in the review literature. At low RH, water molecules fill free volume between polymer chains and help the barrier; the minimum sits at about 20 to 40% RH, and at higher RH plasticisation makes the barrier worse. A ScienceDirect overview of EVOH says it must be sandwiched to protect it from moisture.
That sandwiching works in practice. In a study of EVOH and polyamide shrink bags for beef, the film with two PA blend layers gave the best oxygen barrier of the films tested, which the authors link to the PA layer shielding the EVOH from moisture gain. A published patent application also notes that EVOH loses barrier performance as RH rises beyond 50 to 70 percent.
Our calculation, from the 0 to 85% RH range above: 0.05 / 0.01 = 5, so the EVOH32 permeability coefficient rose about fivefold across that humidity range in the cited data.
Temperature: a 38 C WVTR test is not a 23 C number
The ASABE paper on PE films for modified atmosphere packaging fitted Arrhenius activation energies that averaged 8.73 kcal/mol for O2 and 6.22 for water vapour. That converts to about 36.5 and 26.0 kJ/mol (8.73 x 4.184 and 6.22 x 4.184).
Our calculation, assuming the fit still holds up to 38 C (the paper measured 0 to 23.2 C, so this is an extrapolation): the rate ratio between 38 C (311.15 K) and 23 C (296.15 K) is exp[(Ea / R) x (1/296.15 minus 1/311.15)]. For oxygen, (36 526 / 8.314) x 0.0001628 = 0.715, and e^0.715 is about 2.0. For water vapour, (26 025 / 8.314) x 0.0001628 = 0.510, giving about 1.7. So a PE film’s OTR would roughly double between 23 C and 38 C, and its WVTR rise by around two thirds.
Not every structure behaves this way. In one PE and PP film study, temperature had no definite effect on the OTR of metallised PP. For a quick estimate of a layer stack’s combined barrier, the laminate estimator is the Free tool: it gives an indicative total, which you then check against measured data.
Typical levels, and why sources disagree
A packaging distributor lists normalised OTR ranges for roughly 25 µm film at 25 C and 0% RH: EVOH 0.1 to 0.2, BOPP 1,000 to 2,500, CPP 2,300 to 3,100 and LDPE 7,000 to 8,500 cm3/m2/day. Labthink’s guide gives a similar picture, with PE above 5,000 and EVOH coextruded films below 2 cc/m2 day.
Other compilations differ sharply. A ScienceDirect table lists PE at 70 to 550 cm3 m-2 per day at 20 to 23 C, which is more than an order of magnitude below the distributor’s LDPE range. The excerpt doesn’t show thickness or density for those entries, which is the most likely reason. Until the basis is stated, the two lists can’t be compared.
For WVTR at 38 C and 90% RH, a converter’s guide sorts PET/AL/PE and foil laminations below 0.5 g/m2/day and single-layer PE or PP above 10. Treat such bands as rough orientation. They come from a seller of films, not a standards body.
Material versus package: where lab and shelf life part ways
Film tests miss what a finished pack has: seals, creases, closures and handling damage. F1307 exists for that reason, since it analyses oxygen permeating into a whole packaging system, including pouch or container walls and closure or lidding. High temperature gives higher rates and faster tests, while low temperature gives lower rates and longer tests.
For flex damage, ASTM F392 uses pinhole formation as the failure criterion, though gas transmission can substitute or complement it. If a laminate passes OTR flat and fails shelf life, test it after flexing before blaming the polymer.
Common mistakes
- Comparing a dry (0% RH) EVOH figure with a PET figure measured at 50% RH. The EVOH value will look better than it behaves in humid storage.
- Quoting a film OTR as if it applied to the finished pack, seals and closure included.
- Reading a “less than” supplier figure as a typical value.
- Using a 38 C WVTR as if it were the storage condition.
- Ignoring the test gas: 100% oxygen in the instrument and 20.9% in air are different partial pressures, and some labs run a lower concentration and scale the result (one patent runs 10% oxygen in nitrogen to keep permeation within the detector range).
- Mixing cm3/(m2 day), cc/100 in2/day and per atm versus per bar in one comparison table.
What this means for you
Procurement: ask suppliers for barrier data at your storage condition, with method, edition, temperature, RH and thickness. If they only have 0% RH data for an EVOH or PA structure, ask for a second point and request a quote that includes the test.
R&D and quality: add a flex test and a whole-pack test to the film test, and request rate-versus-time curves so equilibrium is visible. Check the current text of each standard before you cite it.
Students: if two data sheets disagree by 10 times, check thickness and conditions before suspecting either one.
If your project involves recycled content targets or EPR fees tied to barrier structures, the rules differ by market; see ppwreu.org and check the current text.
Sources
- Ametek Mocon: ASTM F1249
- Ametek Mocon: ASTM F1307
- Wikipedia: Oxygen transmission rate
- IHS Markit: ASTM F1307-20
- ASTM F1307-14 scope and significance text
- Taylor and Francis: Recent Updates on the Barrier Properties of EVOH, a Review
- SciELO: Properties of barrier shrink bags made with EVOH and polyamide
- ScienceDirect: Ethylene Vinyl Alcohol overview
- ScienceDirect: Oxygen Transmission Rate overview
- ASABE: Variability in O2, CO2 and H2O transmission rates among commercial polyethylene films
- Packaging Warehouse: OTR Explained
- Labthink: OTR and MVTR Specifications for Barrier Food Packaging
- Myplast: Extend Shelf Life with Barrier Films
- Innovapax: OTR / WVTR Barrier Unit Converter
- USPTO: Patent 9,181,460, Gas transmitting polyurethane adhesive
- USPTO: Patent 7,416,767, Anti-blocking coatings for PVdc-coated substrates
- USPTO: Patent 11,260,633, Multilayer films
- USPTO: Patent 12,036,775, Barrier film
- USPTO: Patent 6,265,038, Transparent high barrier multilayer structure
- Society of Vacuum Coaters: Oxygen and water vapor transmission in ceramic-coated films
- USPTO: Patent 10,858,619, Water-soluble unit dose articles
Values are typical figures from the cited sources. Real performance depends on the grade, the test method and the conditions. Check the supplier's data sheet and test your own structure.
Header image: illustration, AI-generated.